Matthias Grotevent | TU Dortmund: What is the step-by-step route from solubilized sodium stannate to a transparent tin oxide nanocrystal dispersion?
02:37 - 04:31
Other snippets from this talk
Summary of the clip:
What is the step-by-step route from solubilized sodium stannate to a transparent tin oxide nanocrystal dispersion?
Sodium stannate is first solubilized in water. Adding an acid such as acetic acid immediately forms material: crystalline, monodisperse nanocrystals. Shaking ensures acid and water are well mixed. Centrifugation then separates the particles from the solvent. Sodium acetate is a byproduct, so the slightly colored supernatant is discarded; some nanocrystals are lost, but it is pretty much transparent and a lot of mass remains.
The nanocrystals are washed by adding more water and repeating the process, then the water is discarded. Acetic anhydride is added; it hydrolyzes with remaining water trapped between the nanocrystals, consumes it, and creates acetic acid. It also functionalizes the nanocrystal surface with acetate. Over roughly 48 hours, this yields a completely transparent colloidal dispersion; if particles remain and are not dust, wait longer.
A usual wait is one week, and the dispersion can be kept much longer because it does not degrade quickly. Yield was measured after annealing the slurry at 300 degrees Celsius to remove all the water and measuring tin. The route therefore combines acid-driven nanocrystal formation, centrifugation, washing, and acetic-anhydride surface functionalization to produce the final colloidal dispersion.
In this short video, you can learn:
* Adding acetic acid to solubilized sodium stannate forms crystalline, monodisperse nanocrystals, with sodium acetate as a byproduct.
* Centrifugation and water washing remove the solvent and byproduct before acetic anhydride is introduced.
* Acetic anhydride consumes trapped water, creates acetic acid, and functionalizes the surface with acetate, giving a transparent colloidal dispersion after about 48 hours.
๐ **Clip Abstract** Sodium stannate is solubilized in water, an acid such as acetic acid is added, and crystalline monodisperse nanocrystals form; centrifugation and washing remove solvent and sodium acetate byproduct. Acetic anhydride then hydrolyzes trapped water, creates acetic acid, and functionalizes the nanocrystal surface with acetate, producing a transparent colloidal dispersion over roughly 48 hours that can be kept for a week or much longer without quick degradation.
About the speaker:
* Speaker: Matthias Grotevent
* Company: TU Dortmund
* Event: Perovskite Connect 2026 | Berlin
* Location: Estrel, Berlin
Save the date: Perovskite Connect 2027 | 20 and 21 OCT 2027 | Berlin
Co-located with the Future of Electronics RESHAPED conference and exhibition
Learn more: https://www.techblick.com/perovskiteconnect
Intestered in exhibiting: learn more here: https://www.techblick.com/perovskiteconnect
#TinOxideNanocrystals, #SodiumStannate, #AceticAnhydride, #ColloidalDispersion, #PerovskiteSolarCells, #NanocrystalSynthesis
This is a highlight of the presentation:
A Robust Room-Temperature Synthesis of Monodisperse Tin Oxide Nanocrystals for Perovskite Solar Cells
21 and 22 OCT 2026
Estrel, Berlin
Organised By:
More Highlights from the same talk.
00:37 - 02:04
Can a 12-hour, five-chemical tin oxide bath be replaced by a two-chemical, six-minute sodium stannate process?
Can a 12-hour, five-chemical tin oxide bath be replaced by a two-chemical, six-minute sodium stannate process?
The baseline was chemical bath deposition for tin oxide thin films: a water-filled vessel, immersed substrates, a 12-hour reaction, five chemicals and oxygen from air diffusing into the water. To accelerate it, a student proposed sodium stannate. The revised bath used only water and sodium stannate and produced an equally good chemical bath-deposited film in six minutes.
Device fabrication gave decent results, but yield was a concern. Heterogeneous growth on the substrate competed with homogeneous tin oxide growth in solution; that material flocculated out, and some unreacted sodium stannate remained. It worked very well on FTO substrates, not as well on ITO or flexible substrates. That substrate dependence pushed the work toward nanocrystal inks, where a supply-chain issue was also noticed.
The six-minute sodium stannate bath is the central result: a two-chemical route replacing a 12-hour, five-chemical bath plus oxygen, with decent device fabrication. Its limits are explicit: homogeneous precipitation reduces yield, unreacted precursor remains, and performance is substrate-dependent. The contrast between very good FTO results and weaker ITO or flexible results, plus the supply-chain issue seen with nanocrystal inks, defines the next technical questions.
In this short video, you can learn:
* Chemical bath deposition at MIT used water, five chemicals, oxygen from air, and a 12-hour reaction to grow tin oxide thin films.
* Sodium stannate reduced the bath to water plus one chemical and produced an equally good film in six minutes, with decent device fabrication results.
* Yield was limited by homogeneous tin oxide growth and unreacted sodium stannate, and the process worked very well on FTO but not as well on ITO or flexible substrates.
๐ **Clip Abstract** A tin oxide chemical bath deposition process using water, five chemicals, oxygen and a 12-hour reaction was accelerated with sodium stannate to a two-chemical, six-minute bath that gave an equally good film and decent device results. Yield was limited by homogeneous growth and residual unreacted sodium stannate; FTO outperformed ITO and flexible substrates; and the work moved to nanocrystal inks where a supply-chain issue appeared.
About the speaker:
* Speaker: Matthias Grotevent
* Company: TU Dortmund
* Event: Perovskite Connect 2026 | Berlin
* Location: Estrel, Berlin
Save the date: Perovskite Connect 2027 | 20 and 21 OCT 2027 | Berlin
Co-located with the Future of Electronics RESHAPED conference and exhibition
Learn more: https://www.techblick.com/perovskiteconnect
Intestered in exhibiting: learn more here: https://www.techblick.com/perovskiteconnect
#TinOxideThinFilms, #SodiumStannate, #ChemicalBathDeposition, #FTOSubstrates, #PerovskitePhotovoltaics, #NanocrystalInks
10:01 - 11:28
Why did nano cracks on FTO force a double spin-coat, and why did ITO remove hysteresis?
Why did nano cracks on FTO force a double spin-coat, and why did ITO remove hysteresis?
On FTO, nano cracks appeared on the ridges of the crystals, correlating with considerably bad performance. The ink was diluted by a factor of two and spin coated twice, with annealing between coatings, to fill the underlying substrate cracks. This produced a drastic device improvement in the IV curve, though not the best IV curve ever seen.
Because cracks on the ridges were a problem, the work moved to ITO substrates, which are considerably flatter. No such nano cracks were observed there. The IV curve immediately became much better, and there was no hysteresis or less hysteresis without any addition of potassium chloride, which would typically have been added.
For stability, devices were made on the same ITO substrate with tin oxide: one solar cell with a 2D perovskite passivation layer, one without. The unoptimized 2D passivation gave high efficiency but degraded rather fast then seemed to level out. The device without 2D passivation had lower PCE but looked more stable over time, suggesting degradation was more at the hole transporting perovskite interface than at the tin oxide interface.
In this short video, you can learn:
* Diluting the ink twofold and applying two spin-coat/anneal cycles filled FTO ridge nano cracks and drastically improved the device IV curve.
* Moving to flatter ITO eliminated the observed nano cracks and yielded a much better IV curve with no or less hysteresis without potassium chloride.
* Unoptimized 2D perovskite passivation raised efficiency but degraded fast, while the unpassivated device had lower PCE and appeared more stable, pointing to the hole transporting perovskite interface.
๐ **Clip Abstract** Nano cracks on FTO crystal ridges were addressed by halving ink concentration and spin coating twice with annealing, giving a drastic IV improvement. Flatter ITO removed those cracks and enabled better IV with no or less hysteresis without potassium chloride; stability tests with and without 2D perovskite passivation suggested degradation at the hole transporting perovskite interface.
About the speaker:
* Speaker: Matthias Grotevent
* Company: TU Dortmund
* Event: Perovskite Connect 2026 | Berlin
* Location: Estrel, Berlin
Save the date: Perovskite Connect 2027 | 20 and 21 OCT 2027 | Berlin
Co-located with the Future of Electronics RESHAPED conference and exhibition
Learn more: https://www.techblick.com/perovskiteconnect
Intestered in exhibiting: learn more here: https://www.techblick.com/perovskiteconnect
#FTONanoCracks, #DoubleSpinCoating, #PotassiumChloride, #2DPerovskitePassivation, #PerovskiteSolarCells, #Photovoltaics
05:00 - 07:08
Can tin oxide nanocrystal synthesis ignore reaction time, temperature, stirring and injection rate within practical limits?
Can tin oxide nanocrystal synthesis ignore reaction time, temperature, stirring and injection rate within practical limits?
The standard synthesis was evaluated by TM imaging before device results. The reaction was run as fast as two seconds in the lab, or the mixture was left for 20 hours; both gave basically the same results. Within this timeframe, the synthesis is not sensitive to timing, although a nanosecond-scale reaction may leave material not fully reacted.
Stirring was checked and found unnecessary: the solutions need to be mixed a little, but not vigorously stirred. The synthesis was done at room temperature, and at 70 degrees Celsius similar nanocrystal sizes were obtained. The speaker notes surprise that aiming for different sizes always produced the same result, calling this an advantage for scale-up.
Injection of acetic acid was tested by adding it at once versus adding it over about a minute, and both worked. The reaction appears independent of reaction time in the given timeframe, with no real dependence on temperature and reaction speed. It does not matter when the acid is added or how the solutions are mixed, prompting efforts to understand what is happening.
In this short video, you can learn:
* Tin oxide nanocrystal synthesis gave basically the same results after two seconds or 20 hours within the tested timeframe.
* The reaction did not require vigorous stirring and worked at room temperature and at 70 degrees Celsius with similar nanocrystal sizes.
* Adding acetic acid at once or over about a minute both worked, showing no real dependence on injection timing or mixing in the tested range.
๐ **Clip Abstract** A standard tin oxide nanocrystal synthesis for perovskite solar cells was tested across two seconds to 20 hours and remained insensitive to timing within that window. Room-temperature and 70 degrees Celsius syntheses gave similar sizes, vigorous stirring was unnecessary, and acetic acid injection at once or over about a minute both worked.
About the speaker:
* Speaker: Matthias Grotevent
* Company: TU Dortmund
* Event: Perovskite Connect 2026 | Berlin
* Location: Estrel, Berlin
Save the date: Perovskite Connect 2027 | 20 and 21 OCT 2027 | Berlin
Co-located with the Future of Electronics RESHAPED conference and exhibition
Learn more: https://www.techblick.com/perovskiteconnect
Intestered in exhibiting: learn more here: https://www.techblick.com/perovskiteconnect
#TinOxideNanocrystals, #RoomTemperatureSynthesis, #AceticAcidInjection, #ReactionTimeInsensitivity, #PerovskitePhotovoltaics, #ColloidalNanocrystals
About this talk
โ A Robust Room-Temperature Synthesis of Monodisperse Tin Oxide Nanocrystals for Perovskite Solar Cells ยท Matthias Grotevent ยท Perovskite Connect 2026