Alan Brown | Nagase ChemteX: How can you make printed electronics survive 20+ wash cycles?
06:51 - 08:04
Other snippets from this talk
Summary of the clip:
How can you make printed electronics survive 20+ wash cycles?
For wearable electronics to be commercially viable, they must withstand repeated laundering without failing. A primary challenge is maintaining stable electrical resistance after numerous wash cycles. This analysis investigates how the physical construction, or stack-up, of the printed conductive layers directly impacts their durability and longevity when subjected to washing.
The study compares several different ink constructions printed on a TPU substrate, with a target of keeping resistance increase below 150% (a 2.5x change). The configurations tested include a single layer of carbon ink, a single layer of silver ink, a bi-layer structure with carbon ink printed over the silver to act as a protective layer, and finally, a tri-layer "sandwich" structure of carbon-silver-carbon.
The results unequivocally show that the tri-layer carbon-silver-carbon construction provides the most robust performance. While other configurations fail relatively quickly, the tri-layer stack-up comfortably survives 20 wash cycles while staying within the target resistance specification. This demonstrates that encapsulating the primary silver conductor between two layers of carbon ink is a highly effective strategy for creating durable, washable e-textiles.
In this short video, you can learn:
* The critical importance of ink stack-up for durability in e-textiles.
* Comparative performance data for single, bi-layer, and tri-layer conductive ink structures.
* Why a carbon-silver-carbon sandwich structure offers the most robust protection against wash-induced failure.
📋 **Clip Abstract** This clip reveals the significant impact of ink layer construction on the washability of printed circuits for wearables. A tri-layer carbon-silver-carbon stack-up is shown to dramatically improve durability, surviving 20 wash cycles with minimal resistance change.
🔗 Link in comments 👇
#PrintedElectronics, #ConductiveInkStackUp, #WashableElectronics, #CarbonSilverCarbon, #FlexibleElectronics, #WearableElectronics
This is a highlight of the presentation:
My apologies on the delay getting this to you.
More Highlights from the same talk.
05:42 - 08:00
Why can the same stretchable ink fail on one TPU and work on another, and which circuit pattern keeps it conductive?
Why can the same stretchable ink fail on one TPU and work on another, and which circuit pattern keeps it conductive?
Substrate versus stretch comes down to pairing: the right ink combination with the right TPU combination. Many TPUs are on the market and each can perform differently with the same ink, so the starting point is the elongation your application actually needs, then whether the ink meets it. A TPU that appears to stretch further may simply fit different parameters and remain a valid option.
Processing is the next gate. These are conventional screen-printed inks, and general processing runs at 120 to 130 °C to reach optimum resistivity values. The critical parameter is whether the TPU can be processed at those temperatures and maintain dimensional stability. If the TPU is later transferred to a garment or another fabric, the transfer temperature the TPU needs is a further consideration.
Circuit design then changes the stretchability of the ink itself. The straight-line pattern shows the exponential curve of resistance rise, while the sinusoidal and the ohm patterns far outperform on percent stretch versus resistivity. Like a Slinky, those geometries alleviate stress in the pattern and reduce resistance increase as the material stretches further — the earlier CI1036 result was cited as about a 40% significant increase.
In this short video, you can learn:
* Identical ink can perform differently on different TPUs, so the elongation required by the application must be defined before the ink is selected.
* Conventional screen-printed inks need 120 to 130 °C processing to reach optimum resistivity, which makes TPU dimensional stability a critical filter.
* Sinusoidal and ohm-shaped circuit patterns act like a Slinky to alleviate stress and cut the resistance rise under stretch compared with a straight line.
📋 **Clip Abstract** Stretchable e-textile inks are a pairing problem: the same screen-printed ink behaves differently across TPUs, so application elongation, the 120 to 130 °C processing window and garment transfer temperature constrain selection. Sinusoidal and ohm circuit geometries, working like a Slinky, limit the resistance rise a straight-line trace suffers under stretch.
About the speaker:
* Speaker: Alan Brown
* Company: Nagase ChemteX America LLC
* Event: Electronic Textiles RESHAPED 2026 | Berlin
* Location: Estrel, Berlin
Electronic Textiles RESHAPED 2027 | Berlin
📅 Save the date: 20 and 21 October 2027
📍 Berlin, Germany
📋 Info: https://www.techblick.com/electronictextilesreshaped
#ScreenPrintedInk, #ThermoplasticPolyurethane, #SinusoidalCircuitPattern, #DimensionalStability, #ElectronicTextiles, #StretchableElectronics
09:44 - 12:02
Which stack-up survives IEC washing longer: silver-on-carbon, or carbon-silver-carbon, and at what resistance increase?
Which stack-up survives IEC washing longer: silver-on-carbon, or carbon-silver-carbon, and at what resistance increase?
Washability testing tracks resistance change per wash cycle, circuit construction and test temperature. The baseline stack-up places silver on top of carbon; the alternative sandwiches silver between two carbon layers. Testing followed IEC wash standards against a specified target of less than 150% resistance increase, or two and a half times. The construction of the circuit matters, not just the ink.
Initially, only the carbon-silver-carbon tri-sandwich stack-up was successful up to 20 washes, using the current CI1036 material. The next-generation CI1096 material, shown as the bottom blue line, reached up to 50 wash cycles. Both results use a TPU film with carbon, silver, carbon. The sandwiching of silver is important in the circuit construction.
Substrate choice can produce significant performance differences even when moving from one TPU film to another TPU film. Those films have different moisture permeability properties. For wearable washability, the relevant questions include resistance change with each wash cycle, how the circuit is constructed, and the temperature used for testing. Performance over 50 or 100 wash cycles must be assessed against the specified resistance-increase target.
In this short video, you can learn:
* The specified washability target was less than 150% resistance increase, equal to two and a half times.
* The carbon-silver-carbon tri-sandwich with CI1036 was successful up to 20 washes under IEC wash standards.
* The next-generation CI1096 material reached up to 50 wash cycles on TPU film with carbon, silver, carbon.
📋 **Clip Abstract** This clip compares a silver-on-carbon stack-up with a carbon-silver-carbon sandwich for washable electronic textiles. It reports IEC wash testing against a less-than-150% resistance-increase target, with CI1036 reaching 20 washes and next-generation CI1096 reaching 50 cycles, while noting TPU moisture-permeability differences.
About the speaker:
* Speaker: Alan Brown
* Company: Nagase ChemteX America LLC
* Event: Electronic Textiles RESHAPED 2026 | Berlin
* Location: Estrel, Berlin
Electronic Textiles RESHAPED 2027 | Berlin
📅 Save the date: 20 and 21 October 2027
📍 Berlin, Germany
📋 Info: https://www.techblick.com/electronictextilesreshaped
#CarbonSilverCarbonSandwich, #IECWashStandard, #CI1096, #TPUMoisturePermeability, #ElectronicTextiles, #WearableElectronics
07:54 - 09:50
How much does next-generation silver ink reduce resistance rise and recover after repeated stretching?
How much does next-generation silver ink reduce resistance rise and recover after repeated stretching?
The CI1096 is positioned as a next-generation silver ink, benchmarked directly against the CI1036 legacy product on a resistance-versus-stretch chart. Both formulations show very good stretch properties, but the CI1096 delivers less of a change in resistance, which the speaker says makes the design engineer's job easier when laying out stretchable circuits. A second chart shows the newer ink recovering very well as it returns to its original positioning.
Cycle testing shown here covers only five cycles with the CI1096, with a slight increase expected over time. The substrate was Elecom stretch white: 7.44 inches initial length, 7.7 inches final. The speaker stresses the ink is not increasing in resistance greatly — a longer trace from substrate elongation raises resistance slightly anyway, not significantly. This shows very good repeatability of stretch properties under cycling.
The trade-off is explicit: the legacy CI1036 already offers very good stretch properties, but the next-generation CI1096 narrows the resistance change and returns closer to its original positioning after stretching. For designers, that smaller swing makes designing these circuits a little easier. The speaker notes that stretch performance with these inks, particularly as applications get more demanding, remains one of the main areas of focus.
In this short video, you can learn:
* CI1096 shows a smaller resistance change under stretch than the legacy CI1036, while both retain very good stretch properties.
* Five-cycle testing on Elecom stretch white moved substrate length from 7.44 to 7.7 inches, producing only a slight resistance rise.
* Part of the measured resistance increase is geometric, from the longer trace, rather than the ink itself degrading.
📋 **Clip Abstract** The CI1096 next-generation silver ink is compared with the legacy CI1036, showing a smaller resistance change under stretch and strong recovery toward the original position. Five-cycle testing on Elecom stretch white substrate, from 7.44 to 7.7 inches, produced only a slight resistance rise attributed largely to the longer trace rather than ink degradation.
About the speaker:
* Speaker: Alan Brown
* Company: Nagase ChemteX America LLC
* Event: Electronic Textiles RESHAPED 2026 | Berlin
* Location: Estrel, Berlin
Electronic Textiles RESHAPED 2027 | Berlin
📅 Save the date: 20 and 21 October 2027
📍 Berlin, Germany
📋 Info: https://www.techblick.com/electronictextilesreshaped
#SilverInkStretchRecovery, #ResistanceRecovery, #StretchWhiteSubstrate, #FiveCycleStretchTest, #ElectronicTextiles, #StretchableElectronics
Other talks by Alan Brown
- Stretchable, Wearable and Washable Inks: Meeting the Requirements for Next-Generation Electronic Textiles · Electronic Textiles RESHAPED 2026 Berlin
- Conductive Ink Selection for Medical Electronics: Critical Material Properties · TechBlick Innovations Festival July 2026
- Conductive Inks for Medical/ Wearable Electronics · Additive, Printed, Hybrid and Sustainable Electronics Innovations Day 2025
- Next Generation Stretchable Conductive Ink · The Future of Electronics RESHAPED 2025 USA
- Conductive Inks for Wearable/ Stretchable Electronics · The Future of Electronics RESHAPED 2024 Berlin
- Conductive Ink Wash Testing · TechBlick Innovations Festival | Free-To-Attend 2024
- Recent Developments of Conductive Inks for Printed Electronics · Innovations Festival: Printed, Flexible, Hybrid, 3D, Wearable, & Textile Electronics 2023
- Recent Trends of Conductive Inks for Printed Electronics · Printed, Hybrid, InMold, and 3D Electronics 2022
More highlights from Alan Brown
- ▶ Why can the same stretchable ink fail on one TPU and work on another, and which circuit pattern keeps it conductive? · Electronic Textiles RESHAPED 2026 | Berlin
- ▶ How much does next-generation silver ink reduce resistance rise and recover after repeated stretching? · Electronic Textiles RESHAPED 2026 | Berlin
- ▶ Which stack-up survives IEC washing longer: silver-on-carbon, or carbon-silver-carbon, and at what resistance increase? · Electronic Textiles RESHAPED 2026 | Berlin
- ▶ What resistivity ranges and dielectric specs separate silver, carbon and other conductive inks? · The Future of Electronics RESHAPED 2025 | Berlin
- ▶ Why is silver at a 40-year high, and how does a low-silver ink cut cost? · The Future of Electronics RESHAPED 2025 | Berlin
- ▶ Can a low-cost composite ink beat a 100% silver PTF after 1,600 hours and 85/85 humidity? · The Future of Electronics RESHAPED 2025 | Berlin
- ▶ How does the silver-to-binder ratio affect the overall performance of stretchable conductive inks? · The Future of Electronics RESHAPED USA | Boston 2025
- ▶ How does line trace width impact the durability of conductive inks under repeated creasing? · The Future of Electronics RESHAPED USA | Boston 2025
- ▶ What is the impact of a carbon-silver-carbon tri-layer structure on the washability of conductive inks on TPU substrates? · The Future of Electronics RESHAPED USA | Boston 2025